Application and Optimization of Die Casting Technology in New Energy Vehicle Parts Manufacturing

Jul 24, 2025

Leave a message

Currently, die - casting technology is widely used in various fields such as automotive, military, aviation, and medical. The automotive industry holds a significant position in the domestic die - casting parts sector. The rear - drive electric control box main housing is a crucial component in new energy vehicles. The housing comes with its own circulating water chamber and is required to have good mechanical properties and air - tightness. The overall part is relatively small, falling into the medium - and small - sized category. However, the part's structure is relatively complex, and the product has high technical requirements. Only by integrating theoretical development and design in the early stage with actual process improvements in the later stage can qualified products meeting the technical requirements be produced.

 

1.Main Housing Structure and Technical Requirements
The main housing of the electric control box is located in the rear - drive integration of the new energy vehicle. Figure 1 shows its 3D structure. The outline dimensions are 225mm×284mm×79mm, and the weight is 1.24kg. It is a medium and small - sized part with a relatively complex structure. As shown in Figure 2, the overall wall thickness of the casting is about 3mm, with some thicker areas around 8mm. The local rib and deep cavity positions have a wall thickness of around 40mm. At positions with thicker walls, spot cooling is applied to prevent the risk of shrinkage cavities.

The material selected for the main housing part is AlSi12Fe. The part's surface is required to undergo shot blasting treatment. Surface - visible crack defects must not be present. There should be no residual oil or release agent. Oxidation marks are not allowed. The sealing surface, support surface, and the surface for attaching the heat - conductive pad must not have ejector pin marks, scratches, cracks, or burrs. Burrs at the gate or slag pack positions should be less than 0.5mm, and burrs at the parting line and other positions should be less than 0.1mm. Sharp and detachable burrs are not acceptable. For the cavity air - tightness test, the test pressure is 0.5bar, and the leakage rate is 2.5pa/s. For the waterway air - tightness test, the test pressure is 3bar, and the leakage rate is 2.5pa/s.

 

2.Gating and Runner System Design and Numerical Simulation Analysis
With the rapid development of computer technology, die - casting simulation technology has been widely used. This is of great significance for improving the internal quality of castings, shortening the development cycle of castings, and reducing costs.

 2.1 Gating and Runner System Design
The main housing part is a medium - and small - sized part with a relatively complex structure. A one - mold - one - cavity casting system is adopted. Considering the main body's outline and size, and analyzing the filling distance of molten aluminum, the casting system is designed to prevent molten aluminum from directly impacting the core after entering the cavity. The main flow direction should not be aimed at the critical part of the part. The preset casting system of the part is shown in Figure 3. The filling distance of the casting system shown in Figure 3 is the shortest, and the main flow direction of the molten aluminum is directly aimed at the product waterway direction. This ensures the filling quality of the waterway and meets the part's waterway leakage - proof requirements. Two bridges have been added at the filling end to enhance the filling of the molten metal at the end and prevent defects such as cold shutdown and poor molding at the end of the part. Overflow slots are arranged at the end of the metal - filling and the locations initially determined to be prone to air entrapment.

 2.2 Numerical Simulation Analysis
A high - pressure casting simulation of the preset gate and runner system of the part is carried out using simulation software, and the simulation results are analyzed.

2.2.1 Molten Aluminum Filling
As shown in Figure 4, the simulation of the molten aluminum filling process shows that the filling process is smooth. The molten metal from multiple inner gates is well - layered, with no obvious areas of metal collision or convergence. This indicates an ideal filling state of the molten metal.

2.2.2 Filling Time
Figure 5 shows the simulation results of the cavity filling time. It can be seen that the cavity filling time is within 0.2 seconds, which is within a reasonable range.

2.2.3 Gas Pressure Analysis
As shown in Figure 6, the simulation results of the filling gas pressure show that most of the gas is mainly distributed in the overflow slot and the pillar position of the product. Some ribs are used to connect the pillar to enhance exhaust and molten metal filling, ensuring the internal quality of the pillar. A small amount of gas is located in the non - machined areas of the product.

2.2.4 Solidification Analysis
Figure 7 shows the simulation results of the solidification of the molten aluminum at different times. It can be seen that the middle wall - thick position of the product cools slowly and has a risk of shrinkage. Cooling is increased at the corresponding position to ensure consistent solidification of the product. The analysis of the simulation results shows that the preset casting system generally meets the actual production requirements of the part but still has some potential risks. To address the risks associated with problem points, the mold structure and part structure are optimized in advance to prevent defect generation. With this, trial production is carried out. Further optimization of the gate and runner system, part structure, and mold structure based on the actual production status improves the quality of the castings.

 

3.Actual Production
 3.1 Die - Casting Machine Selection
The part's front projection area is 50960mm², and the side core - pulling projection area is 7350mm². Theoretical calculations are carried out based on a safety factor of 1.25, a casting pressure of 75MPa, a slide block wedge angle of 10°, and a ratio of 1.3 for the projection area of the product's additional flow channel and slag pack to the product's front projection area. The resulting mold - opening force is 6300kN, so a 630T die - casting machine is selected for production.

 3.2 Production Process Parameters
Based on the designed die - casting mold for the entire casting and the parameters corresponding to the selected die - casting machine model, theoretical calculations are carried out. When the die - casting machine's plunger moves to 347mm, the molten aluminum just reaches the inner gate position. Therefore, 350mm is set as the theoretical high - speed switching point, and three high - speed switching points of 330mm, 350mm, and 370mm are selected for actual production verification.

 3.3 Actual Production Parameter Verification Results
Figure 8 shows the defects of the products produced at different high - speed switching points. When the high - speed switching point is 330mm, the product has an obvious mold - opening mark at the feeding port. When the point is 350mm, the mold - opening mark at the feeding port is significantly improved. When the point is 370mm, there is no obvious mold - opening mark at the feeding port, but severe gas - hole defects occur at the water - tail position. After verification, the most suitable actual production parameters are as follows: two - fast start position at 350mm, two - fast flow rate at 70%; boost start position at 470mm, and boost flow rate at 60%.

 3.4 Problems Encountered During Actual Production
After verifying three sets of parameters, 200 parts were continuously produced with the final - confirmed parameters. After shot blasting and machining processes, the specific production data of the products is shown in Table 1 (each defect is counted individually, and a product may have multiple defects).

Through statistics, it is found that the main problems of the product are gas holes, leakage, and shot - blasting - induced peeling. In addition, a batch of products experienced molding defects during subsequent production verification, which were resolved on site. The gas holes are mainly located near the sealing groove at the wall - thick position, and are exposed after machining. The leakage occurs due to shrinkage holes between the lower core - pulled waterway hole and the adjacent threaded hole, causing a leak path. The position of the shot - blasting - induced peeling is also identified.

 

4.Improvement of Problem Points
 4.1 Lower Core - pulled Shrinkage Hole
In the first trial production of 200 pieces, 15 pieces were randomly selected for X - ray inspection of internal quality. The results show that each product has shrinkage holes at the blind hole positions. After machining, the blind holes and the lower core - pulled pin holes are interconnected, causing leakage.

Cause analysis: The blind hole is too small to allow the pin to be drawn out, resulting in uneven wall thickness at this position. The local wall thickness is excessive, making it highly susceptible to defects such as porosity and shrinkage holes.

Solutions:

(1) For this position, an additional spot cooling is added to the moving mold, but the improvement of the shrinkage hole is not obvious.

(2) The runner is modified. The shrinkage hole is located at the position filled by the first runner. It is determined that the left half is over - fed. The second runner is blocked and converted into a slag bag. At the same time, the first runner is widened to enhance feeding at the defective position. After the modification, there is some improvement, but leakage products still exist, and other solutions need to be added for improvement.

(3) Local squeezing is added to the lower core - pulled section. In the die - casting industry, local squeezing has a very significant effect on solving shrinkage holes in products, and the technology is quite mature. It is analyzed that there is enough space at the lower core - pulled pin hole position corresponding to the blind hole to set up a squeezing cylinder. Therefore, local squeezing is adopted for the shrinkage hole defect of the blind hole next to the lower core - pulled pin hole.

After changing the squeezing structure, to ensure that the squeezing pin does not stick to the aluminum and affect the squeezing effect, the squeezing pin is set with a core - pulling mist. The squeezing parameters are set to a 2 - second delay, 3 - second pressurization, and overall good cooling of the squeezing pin. There is no residue of water - based release agent at the pin sleeve, and the overall squeezing effect is good. The shrinkage hole defect of the blind hole next to the lower core - pulled pin hole is resolved. As shown in Figure 13, X - rays show no shrinkage holes, and after machining, there is no leakage.

 4.2 Poor Molding of Pillar
After adding the lower core - pullingsqueezing pin, there is a poor molding of a pillar on the product.

Analysis shows that the pillar is located above the product's core - pulled hole. During actual production, the lower core - pulling spray is set. That is, when spraying begins, the lower core - pulled is in the inserted state, which facilitates cooling of the lower core - pulledsqueezing pin. However, with the lower core - pulled in the inserted state during spraying, the water - based release agent will remain in the pillar hole blocked by the lower core - pulled pin. Even with a longer blowing time after spraying, it is difficult to blow away the residual water. The residual water and the over - cooling of the pillar hole are the main reasons for the poor molding defect at this location when the molten aluminum fills the cavity.

Solution: The lower core - pulling spray is canceled, and the lower core - pulled is in the retracted state. Without the obstruction of the core - pulling pin, the residual water in the hole can be blown dry. At the same time, to ensure the spraying and cooling of thesqueezing pin, a longer copper tube is set up to spray thesqueezing pin of the lower core - pulled, and the blowing copper tube for thesqueezing pin is correspondingly lengthened. After implementing the solution, the poor molding defect at this location of the product is resolved.

 4.3 Gas Holes at Thick - Walled Positions of the Product
From the X - ray images, it can be seen that there are gas holes at the thick - walled positions of the product. Some products have gas holes exposed after machining, making them unqualified. Cause analysis: During the filling process of the product, the molten metal converges at this position. The water - tail material supply is insufficient, and the exhaust is not smooth, leading to poor internal quality at this location. The following improvement plans are proposed and verified.

(1) The thickness of the two material - transfer bridges at the water - tail window is increased from 2mm to 3mm to enhance material transfer, but the improvement effect is not obvious.

(2) The three ejector pin holes at the top of the shrinkage hole are changed to cylinder - type ejector pins. The gap between the pin and the pin sleeve is used for exhaust. The defect is somewhat improved, but the improvement is not significant.

(3) A side runner is added to enhance feeding at the defective position. After the first two plans show poor improvement, it is analyzed that the overall feeding on the right side of the product is insufficient. A side runner is added to enhance the overall feeding on the right side.

Under the combined implementation of these three plans, the internal quality of the product at this location is significantly improved. As shown in Figure 19, there are no exposed gas holes after machining.

 4.4 Product Shot - Blasting Peel
Uneven cooling of the product causes flow marks on the product surface, leading to peeling after shot blasting. Cause analysis: The main reason for casting peeling is the special design of certain areas of the casting, with many pillars and grooves. During the filling process of the molten aluminum, there are large fluctuations. When filling at high speed, the molten aluminum flows to places that the mainstream cannot reach, i.e., dead - angle positions. The molten metal splashes, and the temperature drop rate is relatively fast. For the plane areas enclosed by pillars and grooves, heat dissipation is faster, and solidification occurs more quickly. Thus, cold slags, flow marks, or pitting form on the casting surface, which are the main causes of shot - blasting peel. Solutions:

(1) Add material - transfer ribs to enhance the discharge of cold material. Two material - transfer ribs of the same thickness are added at the plane and water - tail positions. This measure improves most of the peeling, but there is still some peeling after shot - blasting at certain positions.

(2) Reasonably control the mold thermal balance. Identify positions with severe flow marks on the product. For positions that cool down quickly on the mold but require cooling, use oil cooling to prevent excessive cooling at these positions. After implementing this measure, the improvement effect is poor, and the peeling state after shot - blasting still exists.

(3) In addition to reasonably controlling the mold temperature, another method to effectively control shot - blasting peel is to add etching to the mold surface. During the flow of molten aluminum in the cavity, if the mold surface is very smooth, etching is performed at positions where the casting is prone to cold slags, flow marks, and pitting. The mold surface becomes uneven with high and low grooves. This disperses the flow direction of the molten aluminum in the cavity and forms an air film between the grooves. This improves the flow of the molten aluminum at this position, avoiding or reducing the generation of cold slags, flow marks, and pitting. After adding etching and verifying shot - blasting, no peeling occurs on the product.

 

5.Conclusion
A multi - pronged approach is necessary to produce high - quality products. Using simulation software for numerical simulation analysis of the casting system of die - casting products in the early stage can effectively identify potential defect risks in actual production. Timely optimization of the casting system or mold structure can narrow down, even avoid or resolve defect risks. Choosing appropriate process parameters can effectively ensure the overall quality of the castings. When actual process parameter adjustments cannot improve product issues, it is essential to consider defect causes from multiple aspects such as casting structure, runner and overflow system, mold cooling, and product structure.
 

Send Inquiry