In - Depth Analysis: Die - Casting Process Optimization for Electrical Control Box Shells

Jul 27, 2025

Leave a message

One,Introduction

Die - casting technology plays a crucial role in modern industrial production and is widely applied in fields like automotive, military, aerospace, and medical industries, with the automotive industry being particularly prominent. The main shell of the rear - drive electrical control box in new energy vehicles is a key component with special structure and performance requirements, making it a focal point in die - casting process research. This article combines theoretical development and practical process improvement to comprehensively explain the die - casting process of electrical control box shells.

 

Two,Main Shell Structure and Technical Requirements

The main shell of the electrical control box is a complex - shaped component in new energy vehicles with a size of 225mm×284mm×79mm and a weight of 1.24kg.

The casting has an overall wall thickness of approximately 3mm, with some thicker areas at 8mm and local rib areas at 40mm, where spot cooling is applied to prevent shrinkage. Made of AlSi12Fe material, it offers excellent casting and mechanical properties for strength and wear - resistance in automotive applications.

The part requires shot - peening for surface roughness and stress - corrosion resistance. Strict requirements include no visible cracks, oil, release agent, or oxidation; defect - free critical surfaces; burrs within specified limits; and leakage - free cavities and waterways under set pressures. These demanding specs pose high challenges to die - casting accuracy.

 

Three,Gating and Runner System Design and Numerical Simulation

Numerical simulation is vital for improving casting quality and efficiency. It helps optimize the gating and runner system, reduces production time and costs, and enhances product quality.

(a) Gating and Runner System Design

For the complex - shaped small - to - medium - sized main shell, a one - cavity - one - mold gating system is used. Considering the part's shape and size, the system is designed to minimize aluminum liquid impact on cores and ensure the main flow direction aligns with key part areas. The design features the shortest possible runner length with the main flow directed toward the product waterway for better waterway filling and leakage prevention. Two bridges are added at the filling end to enhance end - filling and prevent defects like cold shuts and poor formation. Overflow troughs are placed at the metal liquid filling end and potential gas - trapping areas.

(b) Numerical Simulation Analysis

Simulation software is used to analyze the preset gating and runner system.

1. Aluminum Liquid Filling

Results show stable aluminum liquid filling with distinct metal liquid layers at different inner gates and no obvious metal liquid collisions. This indicates a well - designed gating system that ensures orderly filling and lays a solid foundation for high - quality castings.

2. Filling Time

Simulation results show the cavity filling time is within 0.2 seconds, which is reasonable. This short time boosts production efficiency and avoids issues like incomplete filling due to excessive filling time and premature aluminum liquid cooling.

3. Gas Pressure Analysis

Simulation results show most gas is in the overflow trough and product pillar positions. Connecting some pillars with ribs enhances exhaust and metal liquid filling to ensure pillar internal quality. A small amount of gas is in non - machined product areas with less impact on overall performance. The optimized exhaust system effectively expels cavity gas, reducing internal porosity and boosting casting density.

4. Solidification Analysis

Simulation results show the product's central thick - walled area cools slowly, posing a shrinkage risk. Cooling is enhanced at this position to ensure uniform solidification. The preset gating system generally meets production requirements but has some risks. Mold and part structures are optimized early to prevent defects. After trial production, the gating and runner system, part and mold structures are further optimized based on actual production conditions to enhance casting quality.

 

Four,Actual Production

(a) Die - Casting Machine Selection

Based on the part's front projection area of 50960mm² and side core - pulling projection area of 7350mm², and considering a safety factor of 1.25, a casting pressure of 75MPa, a slide block clamping angle of 10°, and a ratio of 1.3 for the additional flow channel and slag pack projection area to the product's front projection area, calculations show a swelling force of 6300kN. Thus, a 630T die - casting machine is chosen for production, with sufficient clamping force and energy to meet the aluminum liquid filling and compaction requirements in the cavity, ensuring casting formation quality.

(b) Process Parameter Determination

Based on the designed die - casting mold and the selected machine, calculations show the aluminum liquid reaches the inner gate when the die - casting machine plunger moves to 347mm. Thus, 350mm is set as the theoretical high - speed switching point, and three points (330mm, 350mm, and 370mm) are chosen for actual production testing to find optimal process parameters.

(c) Actual Production Parameter Verification Results

Results show that at a high - speed switching point of 330mm, the product has obvious mold - opening marks at the feed port, affecting surface and dimensional accuracy. At 350mm, the marks are significantly reduced. At 370mm, there are no marks, but serious gas - porosity occurs at the water tail, causing internal defects. After verification, the optimal parameters are found to be a second - fast start position at 350mm with 70% flow, and an increase - pressure start position at 470mm with 60% flow. These parameters, derived from multiple trials and strict quality inspections, consider the aluminum liquid's flow characteristics, cavity filling and casting solidification, effectively reducing defects and improving production efficiency and quality.

(d) Existing Problems in Actual Production

After continuously producing 200 units with confirmed parameters and completing shot - peening and machining, the collected data (with individual defects counted separately and some products having multiple defects) reveals the following main issues:

1. Porosity: Mainly near the sealing groove of thick - walled areas, some porosity is exposed after machining, affecting casting sealing and mechanical properties. This is due to metal liquid convergence and insufficient exhaust during filling, trapping gas and causing internal porosity.
2. Leakage: Shrinkage at the lower core - pulled waterway hole and adjacent threaded hole causes leakage. The blind hole's uneven thickness and excessive local thickness due to no core - pulling, lead to porosity and shrinkage during solidification.
3. Shot - Peening Peel: Occurs at casting surfaces with flow marks due to uneven cooling, forming cold slags, flow marks or pitted surfaces that peel during shot - peening, impacting surface quality.

Additionally, a batch - formation defect occurred during production validation but was promptly resolved on - site. These issues compromise appearance, dimensional accuracy and performance, risking part failure in actual use. Effective improvement measures are essential.

 

Five,Problem Solutions

(a) Lower Core - Pulling Shrinkage

X - ray inspection of 15 randomly selected units from the first 200 - piece trial production revealed shrinkage in the blind holes, causing leakage after machining. Analysis shows the small blind hole's uneven thickness and excessive local thickness due to no core - pulling, leading to shrinkage.

Solutions:
1. Add excess spot cooling to the moving mold to speed up local metal liquid solidification and reduce shrinkage risk, but results are insignificant.
2. Modify the gating system. The original design caused excessive left - half feeding. The second gating is blocked and replaced with a slag pack, while the first gating is widened to enhance feeding at the defect site, providing some shrinkage improvement but not eliminating leakage.
3. Apply local core - pulling squeeze. Given the lower core - pulling position's sufficient space for a squeeze cylinder, local squeezing is used. After modifying the squeeze structure with spray for the squeeze pin to prevent aluminum adhesion, parameters set as a 2 - second delay and 3 - second pressure application, and ensuring the squeeze pin's overall cooling and no water - based release agent residue at the pin sleeve, X - ray shows no shrinkage and machining confirms no leakage, significantly enhancing casting gas tightness and quality.

(b) Pillar Formation Defects

After adding the lower core - pulling squeeze pin, a pillar formation defect occurs. Analysis reveals the pillar is above the core - pulled hole. During production, lower core - pulling is in the inserted state for spraying, trapping water - based release agent in the pillar hole. Despite prolonged air - blowing, moisture remains, over - cooling the pillar hole and causing filling - related defects.

Solution:
Cancel lower core -pulling spray, retract the core - pulling, and remove the needle obstruction to dry residual water in the hole. To cool the squeeze pin, a long copper tube is used for spraying, with a corresponding longer air - blowing tube. This resolves the pillar formation defect, improving surface and dimensional accuracy.

(c) Porosity in Thick - Walled Areas

X - ray photos show porosity in thick - walled areas, with some exposed after machining. Analysis indicates metal liquid convergence and poor exhaust during filling lead to internal porosity.

Improvement Plans:

1. Increase the thickness of the two over - feed bridges at the water tail window from 2mm to 3mm to boost feeding, but results are insignificant.
2. Replace the three pinholes at the shrinkage top with cylinder - type pins to exhaust gas via the gap between the pin and sleeve, providing some improvement but still insufficient.
3. Add a side gating to enhance feeding at the defect site. Given inadequate feeding on the product's right side, a side gating is added. Together with the first two measures, this significantly improves internal quality, eliminating exposed porosity after machining.

(d) Shot - Peening Peel

Castings with uneven cooling develop flow marks and peel after shot - peening. Analysis shows this is due to special part designs with multiple pillars and grooves. During high - speed filling, aluminum liquid fluctuates, splashes into dead - ends, and cools rapidly. The pillar and groove - enclosed flat areas cool and solidify quickly, forming cold slags, flow marks or pitted surfaces that peel during shot - peening.

Solutions:
1. Add over - feed ribs to enhance cold material discharge. Two additional ribs of the same thickness are placed at the flat and water tail areas, which mostly resolve peeling but not entirely.
2. Adjust mold heat balance by identifying severe flow - mark areas and applying oil - cooling to positions with rapid mold temperature drop yet requiring cooling. However, this yields poor results, with peeling still occurring.
3. Besides mold temperature control, mold surface texturing effectively addresses shot - peening peel. During aluminum liquid filling, textured mold surfaces become uneven, creating air films between recesses that improve aluminum liquid flow and prevent cold slags and pitted surfaces. After texturing, no peeling occurs during shot - peening, significantly enhancing surface quality.

 

Six,Conclusion

In the die - casting process of electrical control box shells, a multi - pronged approach is key to producing high - quality parts. Numerical simulation via software helps identify potential defects early, enabling gating and mold structure optimization and reducing defect risks. Proper process parameter selection ensures casting quality. When parameter adjustments fall short, comprehensive analysis of gating structures, exhaust systems, mold cooling, and part design is necessary.

The implemented optimization measures have greatly improved the die - casting quality of electrical control box shells, effectively resolving issues like porosity, shrinkage, leakage, and shot - peening peel. The castings now meet the high - standards for appearance, dimensional accuracy, and internal quality required by new energy vehicle rear - drive systems. This not only strengthens market competitiveness but also offers valuable practical experience for complex - part die - casting, promoting technological advancement in the industry.
 

Send Inquiry